SureScreen Materials

ISO 17025 UKAS accredited

Over three decades of experience

Stress Corrosion Cracking

Corrosion / Environment

Description

Stress corrosion cracking (SCC), or ‘environmental-sensitive cracking’, is the formation and growth of a crack through a material which is subject to a particular set of conditions. These conditions include the presence of a tensile stress, a corroding medium and a susceptible material. Many alloys are prone to SCC, but the necessary conditions don’t occur that often. This can be dangerous when they do; failure could be unexpected.

Stress corrosion cracking | example 1

SCC in austenitic stainless steel.

One of the earliest cited cases of SCC was a phenomenon termed ‘season cracking’ applied to the brass cartridge cases used by the occupying British forces whilst in India during the nineteenth century. During the monsoon season, the ammunition was stored in horse stables until the dry weather returned. It was apparent that during storage, the cartridges would often crack, and particularly where the case was crimped to the bullet. In 1921 the phenomenon was explained by Moor, Beckinsale and Mallinson, as a combination of the ammonia inherent in the horse urine, and the residual stress that remained in the cold-drawn metal of the cartridges that caused the cracking.

Mechanism

Virtually all metals and alloys are susceptible to SCC under certain conditions that include stress, environment, electrode potential, temperature, contamination, physical damage, or changes in microstructure. Stress may be applied (pressure, thermal, centrifugal, load etc.) or residual (welding, heat treatment, cold work etc). It can be affected by local stress concentrations too (pitting, geometry, microstructure, corrosion product wedging) and by corrosion concentration (evaporation, differential aeration, build up under coatings and in cracks etc). However, most components operate outside the SCC ‘envelope’ either by good fortune or because of some limited understanding of the problem; some materials have a wider ‘envelope’ than others.

One reason SCC can be unpredictable is that it requires a crack initiation stage, but at the start, the growth rate can be slow which means the embryo crack may go unnoticed due to its size; it will be small, tightly closed, and could be filled with corrosion product. It is not unknown for components to resist many thousands of hours of exposure to the corrosive environment with apparently little attack until the embryo cracks develop. Then, growth can be rapid.

SCC occurs when metals are exposed to ‘fluids’ (aqueous, steam, vapour and molten salts). Usually, but not always, temperatures above 50°C are involved too. The all-important initiation stage requires time-dependent changes in either the attacking solution or the metal, through chemical or electrochemical action to locally concentrate the attack at the atomic level. Sometimes, local concentration increases through physical means such as evaporation or localised conductivity changes through the setting up of an electrical cell where different metals or different oxygen levels exist. This cell can also be set up by any discontinuity in the metal surface. It is this variability in initiation conditions that makes SCC rather difficult to predict.

A further factor in SCC is the role of hydrogen, and the effects of hydrogen embrittlement (HE). Many papers on SCC and HE consider these two phenomena as synonymous. Corrosion mechanisms in aqueous environments will generate hydrogen in its atomic form. Depending on the local environment, this hydrogen may be adsorbed into the metal structure and contribute to cracking.

Machining marks and scores (especially poor machining surfaces), generate residual stresses at the surface as well as providing pits and crevices for cells to develop. Lapped and smeared metal seems particularly susceptible to SCC; therefore, machining should be done with appropriate sharp tools and adequate feed rates and cutting speeds. When keyways are cut by milling, avoid smearing or lapping the metal on the sides or corners. Such damage at a machined keyway was thought to be the contributing factor in the failure of a turbine disc at Hinckley Nuclear Power Station in 1969. Controlled experiments have shown that rough surfaces fail by SCC faster than smoother surfaces. This is probably because machining that disturbs the metal more deeply will leave behind higher residual stresses, as it is not uncommon for machining to influence metal several millimetres below the surface, in addition to providing stress concentration points. Often, SCC could be avoided by improved surface finish, and reduced stress concentrations by improved geometry.

Non-metallic inclusions are another source of SCC target. Some types of inclusions are more harmful than others depending on the alloy, due to three significant effects.

  • Firstly, in stagnant conditions the inclusion will affect the local chemistry,
  • Secondly, dissolution of inclusions will leave a pitted surface,
  • Thirdly, sulphides, when attacked chemically will generate hydrogen sulphide locally that removes passive oxide films and forms hydrogen in the surrounding metal leading to HE/Sulphide SCC.

It is thought that manganese sulphide rods that penetrate into the metal provide a much greater reservoir of hydrogen sulphide and hydrogen. Therefore, if there is an option, expose only the plate or bar surface and not the cross section. Also, sulphides that break the surface are more prone to SCC in stagnant conditions due to bacterial attack (Microbial Induced Corrosion).

It has been noted that oxides form preferentially at these sites when temperatures are high enough for oxidation to occur. Iron oxide has a volume that is about twice that of the metal it formed from. As a finger of oxide grows preferentially down the rod-like inclusion, it can result in a process called oxide wedging in which the expanded oxide volume stresses the surrounding metal, leaving it more prone to SCC.

Oxide is also very brittle, so a change in stress can fracture this oxide wedge, resulting in a crevice that exacerbates the situation. This is another reason to avoid end-grain exposure, but it also suggests that low sulphur steels are better than high sulphur steels.

It is not widely appreciated that SCC occurs more readily in metals that are subjected to a very low frequency stress cycle, such as might occur from on/off cycles in a heating system. Furthermore, the severity of SCC will be dependant on the balance between the level of stress and the corrosivity of the environment; a high stress may only need a low level of corrosivity, and correspondingly, a high level of corrosivity would only need a low level of stress for SCC to develop.

SCC may propagate through a metal by intergranular, transgranular, or a combination of both modes.

Intergranular

Attack Intergranular fracture can be identified by smooth facets on the grain boundary surface when examined by electron microscopy. Often, a layer of corrosion product can be seen on the fracture surface, as shown in the image below of a fractured bolt, or the exposed surface may even be darkened and indistinct.

Stress corrosion cracking | example 2

Fracture surface of a high strength steel bolt showing discolouration consistent with light corrosion attack, typical of SCC

Intergranular cracking is common in: carbon steels exposed to caustic, nitrate, acetate and carbonates; low alloy steels with water and steam; sensitised stainless steel and oxygenated water; aluminium alloys and steam or water vapour; beta-titanium alloys exposed to methanol and water; tempered martensitic stainless steels exposed to chlorides (see image below).

Stress corrosion cracking | example 4

SEM image of an area on the bolt shown in the above image revealing intergranular cracking and secondary cracks extending into the surface.

With intergranular attack, the grain boundary is often the preferred route for the crack to grow because in these alloys the grain boundaries and the grains may themselves have slightly different compositions.

An alloy is a mix of one or more metals, and as an alloy solidifies the growing crystals of solid metal in the melt attract a greater proportion of the main elements while the lesser elements are pushed aside into the liquid. As the liquid cools and the crystals grow, they develop a shell of solidifying metal with an increasingly greater proportion of less pure metal, until the last portions to solidify have a much greater level of the alloying elements compared with the metal at the centre of the grains. These last portions to solidify are the grain boundaries. They have a different composition to the grains and some SCC systems prefer them. Some alloys have a wide freezing range and develop this effect to a greater extent. Etching a cross section of these alloys shows the alloy distribution in a pattern known as ‘coring’.

Other alloys have a narrow freezing range and develop less coring. One such alloy, aluminium containing around 12% silicon, has a much narrower freezing range, so it can be cast with thinner cross section without the risk of shrinkage. It probably follows that alloys with a narrow freezing range are less likely to be susceptible to intergranular SCC mechanisms. The Al-12%Si develops two distinct phases. Other alloys that produce distinct phases, like Al-Mg alloys that can develop continuous precipitates of Mg5Al8 generate anodic cells with respect to the matrix. This induces intergranular SCC in chloride solutions.

Transgranular Attack

Transgranular cracks are commonly observed in failure investigations, especially in stainless steel exposed to acidic chlorides, in low strength ferritic steels exposed to acids, in alpha brass exposed to ammonia solutions (although in some conditions, intergranular cracking may develop), in aluminium alloys exposed to chlorides, and in magnesium alloys exposed to dilute fluorides.

Transgranular fractures appear to have cleavage-like facets, with fan-like river markings. There is usually a ‘tunnelling’ effect from side branches that can only be seen on cross sections, though electron microscopy does reveal fissures between grains that have characteristic tunnelling inconsistent with overloading. There is often a tendency to target grain boundaries close to inclusions, with dissolution of the local area through corrosion. Sometimes a coating of corrosion product can be analysed to identify the chemicals responsible.

The theory of tunnelling comes from the mechanism of attack which is thought to develop primarily along planes of atoms; metal grains consist of ordered arrays of atoms, one stacked on top of the other. Artefacts of these planes can be seen as pairs of parallel lines in the microstructure of austenitic stainless steel and brass that have been annealed, when the assembly of stacked atoms generate a ‘stacking fault’ known as a twin boundary.

Transgranular SCC develops from a boundary, stacking fault or locally slipped stack of packed atoms that breaks the surface. The boundary interface is breached by the chemical ions, driven by the electrochemical cell that develops during passivation of the surface. This local attack causes a pit and is accompanied by sliding of the packed atoms over each other, producing a misfit known as a dislocation.

The dislocation is penetrated by the corroding chemical, and the process is repeated. Although the effect usually develops slowly, sometimes cracking propagates at an alarmingly fast rate of minutes or hours, especially worrying when the component may have been operating quite successfully for years previously. On such occasions the term ‘electrochemical knife’ has been used to describe the cleaving open of planes of atoms in a transgranular path.

Appearance

SCC may be observed in different forms, depending on the prevalent conditions and environment. On initial examination affected surfaces may exhibit fine linear cracks or just stain marks although SCC may often initiate at features that render them impossible to observe e.g. from crevices, thread roots, steps in the base of holes etc. Identification of SCC may then be reliant on effective non-destructive testing or microexamination of sections through the component.

The images below show through-thickness SCC that developed from an internal surface, and specifically areas of crevice corrosion.

Outer surface of a stainless steel component showing corrosion staining highlighting the cracks

Outer surface of a stainless steel component showing corrosion staining highlighting the cracks.

Internal surface of the component shown above showing straight SCC and patches of crevice corrosion

Internal surface of the component shown above showing straight SCC and patches of crevice corrosion.

If components can be sectioned for metallurgical examination, SCC may often be readily observed as a network of fine branched cracks such as that shown below.

SCC of stainless steel. Image showing elongated pools of delta ferrite in an austenite matrix, with SCC cracks and corrosion attack around some of the ferrite stringers x500

SCC of stainless steel. Image showing elongated pools (stringers) of delta ferrite (grey horizontal features) in an austenite matrix, with SCC cracks (running vertically) and corrosion attack around some of the ferrite stringers (x500 magnification)

Laboratory analysis of SCC will often include examination by SEM and semiquantitative elemental analysis using the x-ray facility of the SEM (SEM-EDX), particularly when trying to identify what damaging species had contributed to the SCC. For example, SCC of stainless steels is often caused by the presence of chlorides, ions of the element chlorine. SEM-EDX analysis of cracks, and particularly of crack surfaces which have been exposed specifically for the analysis, minimising the potential for contamination, will be particularly interested in identifying the presence of chlorine.

SCC failures of copper alloys, such as brasses, may exhibit varying levels of corrosion damage. This may be observed just as a slight dulling of the brass colour, to significant darkening, dependant on the severity of the corrosion attack. The image below shows such severe darkening indicative of a relatively aggressive environment.

Exposed fracture face of SCC in a brass component showing a highly brittle surface with corrosion staining

Exposed fracture face of SCC in a brass component showing a highly brittle surface with corrosion staining. The crack has originated from the top surface as indicated by the fractographic features and the increased corrosion products

Section through the brass component shown in the image above showing the highly branched cracks x500 Mag

Section through the brass component shown in the image above showing the highly branched cracks (x500 Mag.)

Avoiding Stress Corrosion Cracking

Since stress corrosion cracking is a function of stress, a susceptible material, and a corrosive environment, measures to avoid SCC may focus on one or more of these factors, for example;

  • Avoidance of chemicals or substances that are known to cause and/or accelerate the SCC mechanism.
  • Isolation of the surface of the material from the environment if the environment cannot be changed or controlled.
  • The introduction of shot-peening to introduce compressive stresses in the surface to reduce the potential for crack initiation.
  • Reducing surface damage or irregularities from machining.
  • Controlling the stress levels that a component experiences as well as the correct hardness being achieved can also lower than chances of SCC. Heat treatment to eliminate or reduce residual stress may be beneficial.
  • Modification of design to reduce nominal stress, or areas of stress concentration. • The use and selection of materials resistant to corrosion in the given application.
  • The control of electrochemical potential of the alloy in use to avoid corrosion processes such as may be experienced with cathodic protection.

Examples

Example 1

A 24mm diameter bolt had fractured in service. Examination revealed an unusual fracture that occurred in the head, rather than under the head or in the threads as is typically observed in bolt failures. The fracture followed a concave form within the head, as seen in the image below:

Section through the bolt head showing the concave path of crack propagation

Section through the bolt head showing the concave path of crack propagation.

The unusual form of the fracture follows the general location of highest stress as may be identified in finite element models.

Example 2

A tubular fabrication used in an automotive application failed some weeks after entering service. Investigation identified a crevice at an area of weld lack-of-fusion. This crevice had harboured damaging chemicals from the cleaning and coating processes which resulted in crevice corrosion, from which SCC had then propagated into the cross-section of the tube as shown in the image below. A fatigue crack had then subsequently propagated from the SCC leading to the complete fracture of the tube.

Section through the fracture face of a low carbon steel showing branched stress corrosion cracking extending into the metal x200 Mag

Section through the fracture face of a low carbon steel showing branched SCC extending into the metal (x200 Mag.)

Examples of Stress Corrosion Cracking Associated with Swimming Pools

Since 1985 there have been five incidents of SCC which have led to the catastrophic failure of suspended ceilings in swimming pools, resulting in a combined loss of 56 lives across Switzerland, the Netherlands and Russia, namely:

  • Uster Indoor Swimming Pool (Zurich, Switzerland), 1985.
  • Steenwijk Muncipal Pool (Steenwijk, the Netherlands), 2001.
  • Transvaal Pool (Moscow, Russia), 2005.
  • Dolphin Pool Complex (Chusovoy, Russia), 2005.
  • Zwembad Reeshof Swimming Pool (Tilburg, Netherlands), 2011.

In each of the cases listed above, catastrophic failure occurred leading to the collapse of the suspended ceiling consequentially crushing the people below. Although, this was not the case at Steenwijk as the ceiling collapsed during closing hours of the pool.

In the majority of cases the pools had either fasteners that were made of insufficiently coated carbon steels or were made from austenitic stainless steels which were susceptible to stress corrosion cracking in environments high in chlorides, inherent in the swimming pool environment.

In swimming pools, the chloride production is predominantly generated from disinfectant compounds which are added to the swimming pool water to increase hygiene. Commercially used disinfectant is generally hypochlorous acid and sodium hypochlorite which is known to react in the presence of water with organic materials that are produced by the human users of the pool e.g. sweat, skin particles and urine to form di-chlorine-amine as well as trichlorine-amine which then evaporates from the surface of the pool, concluding in the deposition as condensation on fasteners and roof members, often at high concentrations.

Contact a member of the team

Fields marked with an * are required.